IS 2062 E250 vs E350: How to Choose the Right Structural Steel Grade

IS 2062 E250 vs E350 is one of the most common questions on a structural drawing in India. Both grades come from the same standard, IS 2062:2011, and both are hot rolled structural steel. But they differ in strength, in chemistry and in how easy they are to weld. A wrong choice costs more than steel. It can mean heavier members, failed weld procedures, or rejected material at site.

This guide explains the difference in plain words. It also explains the letters after the grade (A, BR, B0, C), which are often missed on purchase orders. At the end you will find a simple grade line you can copy into your enquiry.

What the numbers mean

In IS 2062, the number after “E” is the minimum yield stress in MPa for thin material (under 20 mm).

  • E250 = 250 MPa minimum yield (under 20 mm)
  • E350 = 350 MPa minimum yield (under 20 mm)

So E350 gives about 40 percent more yield strength than E250 in the same thickness. For a designer, that can mean a lighter section, a thinner plate, or a longer span.

Yield stress falls a little as thickness goes up. This is normal for hot rolled steel, because thick plate cools more slowly in the mill.

Mechanical properties side by side

Values from IS 2062:2011, Table 2 (minimum values).

GradeTensile strength (MPa)Yield under 20 mm (MPa)Yield 20-40 mm (MPa)Yield over 40 mm (MPa)Elongation (%)
E25041025024023023
E27543027526525522
E30044030029028022
E35049035033032022
E41054041039038020

Note how E250 has the highest elongation. It stretches more before it breaks. That is useful for parts that are bent, formed or punched in the shop.

Chemistry and carbon equivalent

Strength is only half the story. The other half is how the steel behaves when you weld it. Engineers use the carbon equivalent (CE) to judge this:

CE = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15

A higher CE means a harder heat-affected zone next to the weld, and a higher risk of cold cracking if the weld is not done right.

Ladle analysis limits from IS 2062:2011, Table 1 (maximum values, percent):

GradeQualityCMnSPSiCE max
E250A0.231.500.0450.0450.400.42
E250BR, B00.221.500.0450.0450.400.41
E250C0.201.500.0400.0400.400.39
E350A, BR, B00.201.550.0450.0450.450.47
E350C0.201.550.0400.0400.450.45
E410A, BR, B0, C0.201.600.045 (C: 0.040)0.045 (C: 0.040)0.450.50

What this means in practice:

  • E250 has a low CE. In normal thickness it welds easily, often with no preheat.
  • E350 gets its extra strength mainly from more manganese and, in many mills, small additions of niobium, vanadium or titanium. Its CE is higher, so thick E350 often needs preheat and low-hydrogen consumables. Your welding procedure (WPS) should decide this, based on CE, thickness and joint restraint.
  • Always ask for the actual CE of each heat on the test certificate, not just the maximum from the standard. Two E350 heats can weld very differently.

The letters that matter: A, BR, B0 and C

The letter after the grade is the sub-quality. It tells you about toughness (resistance to brittle fracture) and how the steel was made.

Sub-qualityCharpy impact testDeoxidationTypical use
ANot requiredSemi-killed or killedGeneral fabrication, static loads, indoor structures
BR27 J at room temperature (25 ± 2 °C)Semi-killed or killedWelded structures with normal service
B027 J at 0 °CSemi-killed or killedOutdoor structures, bridges, cranes, cold nights
C27 J at -20 °CKilledDynamic or fatigue loads, low temperature, heavy welded sections

(For E410, the B0 and C values are 25 J.)

Two more points:

  • For E250 C in 12 mm and above, IS 2062 also calls for a Y-groove crackability test. It checks that the plate will not crack when welded under restraint.
  • “Killed” steel is fully deoxidised. It is more uniform through the thickness, which helps when a plate is welded or loaded across its thickness.

A common mistake is to write only “IS 2062 E250” on the order. Most suppliers will read that as E250 A, which has no impact test. If your structure is welded and outdoors, that may not be what your designer meant.

E250 or E350: a simple way to decide

Choose E250 when:

  • The design is governed by stiffness or deflection, not strength. Extra strength will not help here, because both grades have the same stiffness (Young’s modulus about 200 GPa).
  • The part is heavily bent, formed or punched.
  • Welding is done by a general fabricator and you want the widest weld window.
  • Sections are thin and the load is static.

Choose E350 when:

  • The design is governed by strength, and a lighter section saves weight in the whole structure (columns, long-span beams, crane girders, transmission and telecom towers, trailer chassis).
  • Transport or erection weight matters.
  • The fabricator has qualified welding procedures for higher CE steel.

Consider E410 or above only when your designer has a clear strength case and the fabricator is ready for tighter welding control.

Equivalent grades for export drawings

Export buyers often ask for an IS grade against an EN or ASTM grade. The grades below are near in yield strength. They are not identical in chemistry, testing or thickness bands, so always check the full standard before you substitute.

IS 2062:2011EN 10025-2 (nearest)ASTM (nearest)
E250 BRS235JR / S275JRA36
E250 B0S275J0A36 (with supplementary impact test)
E350 B0S355J0A572 Grade 50
E350 CS355J2A572 Grade 50 (with impact test at -20 °C)

What to check on the test certificate

When rolled steel arrives, check these lines on the certificate against your order. Our guide to EN 10204 test certificates explains the certificate types in detail.

  1. Standard and edition: IS 2062:2011.
  2. Grade and sub-quality: for example E350 B0, not just E350.
  3. Heat (cast) number: it must match the number stamped or painted on the plate.
  4. Ladle analysis with actual CE.
  5. Tensile, yield and elongation for the right thickness band.
  6. Charpy impact values at the right temperature (BR, B0 or C).
  7. Thickness and size of the product tested.

A grade line you can copy

Write your order line like this, so nobody has to guess:

“Hot rolled steel plate to IS 2062:2011, Grade E350 B0, killed, 20 mm thick. Charpy 27 J min at 0 °C. Actual CE to be reported, max 0.45. Test certificate per heat, heat number marked on each plate.”

Change the grade, sub-quality, thickness and CE limit to suit your design.

Send your drawing for a technical review

Not sure which grade or sub-quality your part needs? Send your drawing, the service conditions and the welding route to info@alloynex.com, or use the enquiry form. Our metallurgy team will review it and reply by email.

Related: Rolled steel products | IS 2062 vs IS 1079 | Steel tubes and pipes

FAQ

Is E350 stronger than E250?

Yes. E350 has a minimum yield of 350 MPa against 250 MPa for E250 (under 20 mm thickness), and a minimum tensile strength of 490 MPa against 410 MPa.

Is E350 harder to weld than E250?

It needs more care. E350 has a higher carbon equivalent (up to 0.47 against 0.42 for E250 A), so thick sections often need preheat and low-hydrogen consumables. Follow a qualified welding procedure.

What is the difference between E250 BR and E250 B0?

Both need 27 J in the Charpy impact test. BR is tested at room temperature. B0 is tested at 0 °C, so it gives more confidence for outdoor structures in cold weather.

What is the old name of E250?

Before the 2011 revision, E250 was commonly called Fe 410 W. Use the new designation on all new orders.

Is IS 2062 E350 the same as S355?

They are close in strength but not identical. E350 B0 is near S355J0 and E350 C is near S355J2. Check chemistry, impact temperature and thickness bands before you substitute one for the other.

What should I write on a purchase order for IS 2062 steel?

Write the standard and edition, the grade with sub-quality (for example E350 B0), thickness, impact test temperature, any CE limit, and the certificate you need per heat.