Heat treatment of castings means heating a cast part to a set temperature, holding it there, and then cooling it in a controlled way to change its structure and properties. It is used to relieve stress, improve machinability, raise strength or toughness, and make the part meet the grade on the drawing.
This guide explains the main heat treatment processes for iron and steel castings in simple words. You will learn what each process does, when it is used, and what to write on your drawing or purchase order. It is written for OEM engineers, QA heads and buyers.
Why Heat Treatment of Castings Matters
When a casting cools in the mould, different parts cool at different speeds. Thin walls cool fast and thick sections cool slowly. This can leave internal stress, uneven hardness and a grain structure that is not ideal for the job.
Heat treatment brings the structure under control. Done right, it gives the casting the strength, toughness, hardness and stability the design needs. Done wrong, or skipped, it can lead to cracking, distortion during machining or early failure in service.
The Main Heat Treatment Processes
1. Stress relieving
The casting is heated to a moderate temperature, held, and cooled slowly. This reduces internal stress from casting, welding repair or rough machining. It helps the part keep its shape during final machining and in service. It is common for grey iron machine bases and welded or repaired steel castings.
2. Annealing
The casting is heated to a higher temperature and cooled very slowly, often inside the furnace. Annealing makes the metal softer and easier to machine, and it makes the structure more uniform. In SG iron, annealing is used to produce a ferritic structure with high elongation and good toughness.
3. Normalising
The casting is heated above its critical temperature and then cooled in still air. Normalising refines the grain and gives a good balance of strength and toughness. It is very common for carbon steel castings. In SG iron, normalising gives a pearlitic structure with higher strength and hardness.
4. Hardening and tempering (quench and temper)
The casting is heated, then cooled fast in water, oil or polymer (quenching) to make it hard. It is then reheated to a lower temperature (tempering) to reduce brittleness and reach the required toughness. This is used for alloy steel castings that need high strength and wear resistance, such as gears, rollers and heavy-duty parts.
5. Solution annealing
Used mainly for stainless steel castings. The part is heated to a high temperature and cooled fast to dissolve unwanted phases. This restores corrosion resistance and toughness.
Which heat treatment should you ask for? A decision matrix
| If your casting must… | Ask for this condition | Check on the certificate | Watch out for |
|---|---|---|---|
| Hold its size during machining (grey iron bases, housings) | Stress relieved | Hardness, chemistry | Skipping it on long, thin parts can cause movement |
| Bend before it breaks (SG iron SG 400/15) | Annealed (ferritising) | Tensile, elongation, nodularity | Low elongation if the anneal is short |
| Carry more load and resist wear (SG 600/3, SG 700/2) | Normalised, if not reached as cast | Tensile, hardness | Hardness too high for easy machining |
| Be tough and weldable (carbon steel, IS 1030 W grades) | Normalised, or normalised and tempered | Tensile, elongation, hardness | A coarse as-cast grain if heat treatment is skipped |
| Reach high strength and wear life (alloy steel) | Quenched and tempered | Tensile, hardness, impact if specified | Cracks if the quench is too severe for the section |
| Resist corrosion (stainless steel CF8, CF8M) | Solution annealed | Chemistry, hardness | Slow cooling that reduces corrosion resistance |
Exact temperatures and times depend on the grade, section thickness and the standard you follow. Your foundry sets these in its heat treatment procedure.
Heat Treatment for Iron vs Steel Castings
Grey iron is often used as cast. When needed, it is stress relieved for dimensional stability or annealed for easier machining.
SG iron responds well to heat treatment. Annealing gives a ferritic grade with more elongation. Normalising gives a pearlitic grade with more strength. Read more in our guide on SG iron vs grey cast iron.
Carbon and alloy steel castings almost always need heat treatment. The as-cast structure of steel is coarse, so normalising, or quench and temper for alloy grades, is used to reach the required mechanical properties. See steel vs alloy steel castings for how the grade affects this choice.
Problems That Good Heat Treatment Prevents
- Distortion or movement during machining because of locked-in stress
- Hard spots that damage cutting tools
- Low toughness or brittle behaviour under impact
- Failing tensile, elongation or hardness tests
- Cracks during service under load or temperature change
Heat treatment does not fix every problem. It cannot remove porosity, shrinkage or inclusions. Those are controlled in the casting process itself. Our guide on common casting defects explains how foundries prevent them.
What Buyers Should Specify
Clear instructions avoid confusion later. On your drawing or purchase order, include:
- The material grade and the standard it follows
- The heat treatment condition required, such as normalised, or quenched and tempered
- The mechanical properties to be met, such as tensile strength, elongation and hardness
- Where hardness should be checked on the part
- Whether test bars must be heat treated with the castings
- The test certificates you need with each batch
To learn about the casting and supply work we do, see our services page.
FAQs
Do all castings need heat treatment?
No. Many grey iron castings are used as cast. Most steel castings, and many SG iron grades, need heat treatment to reach their required properties.
What is the difference between annealing and normalising?
Both heat the casting to a high temperature. Annealing cools it very slowly, often in the furnace, to make it softer. Normalising cools it in still air to give a finer grain and higher strength.
Why is tempering done after quenching?
Quenching makes steel very hard but also brittle. Tempering reheats it to a lower temperature to reduce brittleness and reach the right balance of strength and toughness.
Can heat treatment remove casting defects?
No. Heat treatment changes the metal structure, but it cannot close holes, shrinkage or inclusions. Those must be prevented during casting.
How do I know the heat treatment was done right?
Check the test results on the material test certificate, such as tensile strength, elongation and hardness, against your drawing. You can also ask for the heat treatment record for the batch.
Where can I buy heat treated castings in Jaipur?
Alloynex Foundries, Jaipur, supplies grey iron, SG iron, steel and alloy steel castings to drawing, with heat treatment as the part needs. Tell us the grade, the condition you need, such as normalised or quenched and tempered, and the properties to test. Ask for the test results on the certificate for each lot.
| Material | Common heat treatment | What to check on the certificate |
|---|---|---|
| Grey iron | As cast or stress relieved | Hardness, chemistry |
| SG iron | Annealed or normalised | Tensile, elongation, nodularity |
| Carbon steel | Normalised | Tensile, elongation, hardness |
| Alloy steel | Quenched and tempered | Tensile, hardness, impact if needed |
Read steel vs alloy steel castings, SG iron vs grey cast iron and casting defects, or send your drawing to info@alloynex.com.
What should I write on my drawing for heat treatment?
Write the grade and standard, the heat treatment condition, the mechanical properties and the tests and certificate you need.
Can Alloynex supply machined castings?
Tell us at the drawing review if your part needs machining or heat treatment, and we will confirm the supply condition in writing.
जयपुर में हीट ट्रीटेड कास्टिंग कहाँ मिलती है?
एलॉयनेक्स फाउंड्रीज़, जयपुर, ड्रॉइंग के अनुसार ग्रे आयरन, एसजी आयरन, स्टील और अलॉय स्टील कास्टिंग हीट ट्रीटमेंट के साथ सप्लाई करती है। संपर्क: info@alloynex.com
Last updated: 12 November 2026
Get Expert Advice on Your Casting
Not sure which heat treatment your part needs? Share your drawing, grade and service conditions with our team, and we will help you choose the right route.
Send your drawing for a technical review or request a metallurgy consultation: email info@alloynex.com or visit our contact page.
Related: machining allowance on castings
Related: castings for Udaipur plants
Which heat treatment does each casting grade need?
Heat treatment of castings means heating a cast part to a set temperature, holding it and cooling it in a controlled way to change its strength, hardness, toughness or stress level. The right cycle depends on the grade: stress relief for grey iron, annealing or normalising for SG iron and steel, and quench and temper for high strength.
Grade-by-grade heat treatment table (general education)
| Material and grade | Usual heat treatment | Main purpose |
|---|---|---|
| Grey iron, IS 210 FG 200 / FG 260 | Stress relief | Stable size during machining |
| SG iron, IS 1865 SG 400/15 | Ferritising anneal | High elongation and toughness |
| SG iron, SG 600/3 / SG 700/2 | Normalising (if not as-cast) | Higher strength and wear life |
| Carbon steel, ASTM A216 WCB | Normalise, or normalise and temper | Refined grain and toughness |
| Cr-Mo steel, ASTM A217 WC6 / WC9 | Normalise and temper | Strength at high temperature |
| High manganese steel, IS 276 | Water toughening | Tough, work-hardening structure |
| Stainless steel, CF8 / CF8M | Solution anneal | Corrosion resistance |
Numbered checklist to verify heat treatment
- Ask for the furnace time-temperature chart for the lot.
- Ask for a test bar heat treated with the parts.
- Check hardness on each lot against the drawing.
- Ask for a microstructure check where it matters.
- Make sure the certificate names the heat treatment done.
Glossary
- Soaking: holding the part at temperature so it heats through.
- Austenitising: heating steel high enough to change its structure before cooling.
- Quench: fast cooling in water, oil or polymer.
- Temper: reheating after quench to add toughness.
What heat treatment does high manganese steel need?
High manganese steel is usually water toughened: it is heated and then quenched in water. This gives a tough structure that hardens on the surface when it is hit in service.
What heat treatment is used for SG 400/15?
SG 400/15 is often given a ferritising anneal so it reaches high elongation and toughness. Some foundries reach the grade as-cast; the drawing should state if annealing is required.
एसजी आयरन कास्टिंग की हीट ट्रीटमेंट कब ज़रूरी है?
SG 400/15 जैसे ज़्यादा इलांगेशन वाले ग्रेड के लिए अक्सर एनीलिंग, और SG 600/3 या SG 700/2 जैसे ज़्यादा मज़बूत ग्रेड के लिए नॉर्मलाइज़िंग की जाती है, अगर ग्रेड as-cast नहीं मिलता। ड्रॉइंग पर ग्रेड और हीट ट्रीटमेंट लिखें। एलॉयनेक्स फाउंड्रीज़, जयपुर। ईमेल: info@alloynex.com
Related: steel vs alloy steel castings, SG iron vs grey cast iron and cast iron foundry for Kota buyers. Request a metallurgy consultation: info@alloynex.com.
Last updated: 13 November 2026
Further reading: which IS 1865 SG iron grades need annealing or normalising and the castings sourcing checklist for buyers in India.
Related: how heat-treatment condition appears on an EN 10204 3.1 or 3.2 certificate
Related: normalizing vs annealing steel castings: which to choose and grey iron vs SG iron for pump and valve body castings
Related: heat-treated steel castings for Pali textile and Jalore granite units
Related: heat-treated steel castings for Dungarpur and Sawai Madhopur buyers
Related: IS 1030 steel casting grades: N vs W, grade table and how to specify the heat-treated condition
Related: heat-treated WC6 and IS 276 castings for Sikar and Beawar buyers and SG iron castings for Pali: IS 1865 grades
Heat treatment of castings: myths vs facts
Short answer: Heat treatment changes the microstructure of a casting, not its shape. Steel castings to IS 1030 are normally supplied normalized, or normalized and tempered; grey iron is often stress relieved; SG iron is used as-cast or annealed or normalized to reach its IS 1865 grade. The right cycle depends on grade, section size and service.
| Myth | Fact |
|---|---|
| All castings need heat treatment. | Many grey iron castings are used as-cast. Steel castings almost always need normalizing or annealing to refine the coarse as-cast grain. |
| Heat treatment fixes porosity and cracks. | No. Heat treatment cannot close shrinkage or gas holes. Soundness comes from design, feeding and melting. |
| Annealing and normalizing are the same. | Both heat above the critical range, but annealing cools in the furnace (softer) and normalizing cools in still air (finer grain, higher strength). |
| Stress relief changes grey iron strength. | A proper stress relief, below the critical range, mainly reduces distortion after machining; tensile grade stays the same. |
| Harder is always better. | Higher hardness can mean lower toughness and poor machinability. Specify the hardness range the part needs. |
| The test bar proves the casting. | A separately cast bar shows the melt and the cycle. Thick sections may differ; ask for hardness on the casting itself where it matters. |
Quotable fact: a heat treatment chart with time, temperature and cooling method, tied to the heat number, is the simplest proof that the cycle was done. Alloynex Foundries, Harmada, Jaipur, reviews heat treatment needs for buyers in Rajasthan and across India.
Related: SG iron castings for Khairthal-Tijara | normalizing vs annealing steel castings | common casting defects
Send your drawing for a technical review: info@alloynex.com. Last updated: 15 Nov 2026
Worked example: choosing the heat treatment for a steel valve body casting
Short answer: a carbon steel valve body that must pass tensile, impact and pressure tests is usually normalized and tempered; a grey iron gear housing that must hold size after machining usually gets only a stress relief. The part duty decides the route, and the route is written on the drawing.
Case: carbon steel valve body, IS 1030 grade, pressure tested
- Read the drawing: grade, test pressure, impact test (yes/no), machined bores.
- As-cast steel has a coarse structure, so impact values can be low.
- Normalize: heat above the upper critical range, hold by section size, cool in still air. Grain becomes finer and more even.
- Temper if hardness or residual stress must come down after normalizing.
- Test bars go through the same furnace load as the castings.
- Record furnace chart, hold time and test results on the certificate.
Same method, three other parts
| Part | Material | Usual route | Main reason |
|---|---|---|---|
| Gear housing | Grey iron FG 260 | Stress relief | Hold bore size after machining |
| Hydraulic body | SG iron 500/7 | As-cast or ferritize if more elongation is needed | Meet elongation on drawing |
| Crusher liner | Alloy steel | Harden and temper | Wear resistance with toughness |
Quotable fact: normalizing cools the casting in still air, while full annealing cools it slowly in the furnace, so normalized steel is usually a little stronger and harder.
Related: SG iron vs grey cast iron, textile machinery castings for Bhilwara, normalizing vs annealing.
Send your drawing for a technical review, or request a metallurgy consultation, at info@alloynex.com.