Quick answer: ISO 8062-3 sets how much a raw casting may vary from its drawing size, using DCTG grades 1 to 16. Grey iron, SG iron and steel sand castings usually hold DCTG 8 to 12 when machine moulded in repeat runs and DCTG 11 to 14 when hand moulded. Write one note on the drawing, for example “ISO 8062-3 – DCTG 11 – RMA 5 (RMAG H)”.
This guide explains, in simple words, what the grades mean, which grades are normal for sand castings in grey iron, SG iron and steel, and how to write the tolerance note so that the foundry, the machine shop and your incoming inspection all read the drawing the same way.
What is ISO 8062-3?
ISO 8062-3 covers dimensional and geometrical tolerances and machining allowances for castings. It replaced the older ISO 8062:1994, which used “CT” grades, and was first issued in 2007 with a revision in 2023. The older CT grades and the newer DCTG grades use the same numbers, so “CT 10” on an old drawing is read as DCTG 10 today.
The standard gives three things that matter to a buyer:
- DCTG – the total permitted size band for a raw cast dimension.
- RMA and RMAG – the extra metal left on each face that will be machined. See our detailed guide to machining allowance on castings.
- Typical grades for each casting process and metal, so the buyer does not ask for a grade the process cannot hold.
What do DCTG grades mean?
A DCTG grade is a number from 1 (tightest) to 16 (widest). The table value is the total tolerance band in millimetres. For a symmetrical tolerance, split it in half: a band of 4.0 mm means ±2.0 mm. The band grows with the nominal size of the dimension, so a long dimension gets a wider band than a short one in the same grade.
Linear casting tolerances for common sand casting grades (total band, mm)
| Nominal size (mm) | DCTG 8 | DCTG 9 | DCTG 10 | DCTG 11 | DCTG 12 |
|---|---|---|---|---|---|
| up to 10 | 1.0 | 1.5 | 2.0 | 2.8 | 4.2 |
| over 10 to 16 | 1.1 | 1.6 | 2.2 | 3.0 | 4.4 |
| over 16 to 25 | 1.2 | 1.7 | 2.4 | 3.2 | 4.6 |
| over 25 to 40 | 1.3 | 1.8 | 2.6 | 3.6 | 5.0 |
| over 40 to 63 | 1.4 | 2.0 | 2.8 | 4.0 | 5.6 |
| over 63 to 100 | 1.6 | 2.2 | 3.2 | 4.4 | 6.0 |
| over 100 to 160 | 1.8 | 2.5 | 3.6 | 5.0 | 7.0 |
| over 160 to 250 | 2.0 | 2.8 | 4.0 | 5.6 | 8.0 |
| over 250 to 400 | 2.2 | 3.2 | 4.4 | 6.2 | 9.0 |
| over 400 to 630 | 2.6 | 3.6 | 5.0 | 7.0 | 10.0 |
Values are as commonly published from ISO 8062-3 for linear dimensions. Always confirm against your own licensed copy of the standard before you release a drawing.
Quick example: a 120 mm as-cast dimension at DCTG 11 has a total band of 5.0 mm, so the raw casting may measure 117.5 mm to 122.5 mm. At DCTG 9 the same dimension would be 120 ± 1.25 mm.
Which DCTG grade suits sand castings?
The grade a foundry can hold depends on the moulding method and on whether the job is long-series (repeat production) or short-series. Asking for a tighter grade than the process can hold only adds rejection and cost. These are the typical ranges given for sand castings:
- Machine moulded or shell moulded, repeat (long-series) parts? Choose DCTG 8 to 12 for steel, grey iron and SG (ductile) iron.
- Hand moulded, repeat (long-series) parts? Choose DCTG 11 to 14 for all three metals.
- Hand moulded in chemically bonded sand, short-series? Choose DCTG 12 to 14 for steel and DCTG 11 to 14 for grey iron and SG iron.
- Hand moulded in clay-bonded (green) sand, short-series? Choose DCTG 13 to 15 for all three metals.
- Wall thickness? Use one grade coarser than your general grade (for grades up to DCTG 15).
- Still unsure? Start from the coarser end of the range and give a tighter value only to the dimensions that need it. Send the drawing for a technical review before pattern work starts.
Two rules buyers often miss. First, for wall thicknesses the standard applies one grade coarser than the general grade (for grades up to DCTG 15). Second, a dimension that crosses the parting line or depends on a core usually varies more than a dimension inside one mould half, so put tight values only where the function needs them.
How are RMA and DCTG used together?
Machining allowance is added to each machined face, and the casting tolerance sits on top. For an outside dimension machined on both sides, the raw casting size is: R = F + 2 × RMA + DCT/2, where F is the finished size. For a bore machined on both sides it is R = F − 2 × RMA − DCT/2. This makes sure that even a casting at the bottom of its tolerance band still cleans up fully.
RMA is chosen from the greatest overall dimension of the whole casting and an RMA grade from A to K. Sand cast iron parts commonly use grades in the E to H range, while hand-moulded steel parts often need G to K, because steel shows more surface scale and decarburisation.
How do buyers specify casting tolerances on a drawing?
Follow these steps so the note is clear and checkable:
- Pick the general grade from the process table above, matched to your moulding route and order size.
- Write one general note in the title block, for example: General tolerances ISO 8062-3 – DCTG 11 – RMA 5 (RMAG H).
- Mark only critical dimensions with their own tolerance, and leave the rest to the general note.
- Mark datum points (targets) for first machining, so the foundry and machine shop measure from the same places.
- Show machined faces clearly, so the allowance goes only where it is needed.
- State draft and fillet radii or allow the foundry to add them; draft is separate from the tolerance.
- Agree first-off inspection – a dimensional report on the first casting against the drawing before lot supply.
DCTG vs ISO 2768: what is the difference?
| Point | ISO 8062-3 (DCTG) | ISO 2768 general tolerances |
|---|---|---|
| Applies to | Raw cast dimensions | Machined features |
| Typical sand casting band, 100 mm | about 2.5 to 7.0 mm total (DCTG 9 to 12) | ±0.15 mm (class m) |
| Set by | Casting process and metal | Machining process |
| Where on drawing | General casting note | General machining note |
| Use both? | Yes – one for as-cast faces, one for machined faces | Yes |
Using a machining tolerance on an as-cast face is a common drawing error. It makes the casting look out of tolerance even when it is a good part.
Frequently asked questions
What does DCTG stand for?
Dimensional casting tolerance grade. It is a number from 1 to 16 in ISO 8062-3. A higher number means a wider permitted band.
Is CT 10 the same as DCTG 10?
Yes. CT grades come from the older ISO 8062:1994. ISO 8062-3 renamed them DCTG and kept the same numbering.
What DCTG grade is normal for a grey iron sand casting?
Machine-moulded repeat parts usually hold DCTG 8 to 12. Hand-moulded parts usually sit at DCTG 11 to 14.
Are the DCTG values plus-minus?
No. The table gives the total band. Split it in half for a symmetrical tolerance, so 4.0 mm means ±2.0 mm.
ISO 8062-3 में DCTG का क्या मतलब है?
DCTG यानी डाइमेंशनल कास्टिंग टॉलरेंस ग्रेड। यह 1 से 16 तक का नंबर है। टेबल में दिया मान कुल बैंड है, जैसे 4.0 mm का मतलब ±2.0 mm।
ड्रॉइंग पर कास्टिंग टॉलरेंस कैसे लिखें?
टाइटल ब्लॉक में एक सामान्य नोट लिखें, जैसे “General tolerances ISO 8062-3 – DCTG 11 – RMA 5 (RMAG H)”, और केवल ज़रूरी डाइमेंशन पर अलग टॉलरेंस दें।
Send your drawing for a technical review
Alloynex Foundries, Harmada, Jaipur, makes grey iron, SG iron, steel and alloy steel castings to customer drawings for buyers in Rajasthan, across India and for export. At the drawing review we check the tolerance grade, machining allowance, draft and datum points before pattern work starts. Read our castings buyer guide for Rajasthan, see our casting services, or send your drawing for a technical review at info@alloynex.com.
Last updated: 14 November 2026
Related: shrinkage porosity and casting defects: causes and prevention and EN 10204 3.1 vs 3.2 test certificates
Related: SG iron castings for Sikar and Churu: IS 1865 grades
DCTG decision matrix: which ISO 8062-3 grade fits your process and metal?
Quick answer: The achievable casting tolerance grade (DCTG) depends mainly on the moulding process, then on the metal and batch size. Hand-moulded sand castings usually sit around DCTG 11 to 14, machine-moulded or shell castings around DCTG 8 to 12, and investment castings around DCTG 4 to 6. Confirm the grade at drawing review.
| Process | Steel castings | Grey iron | SG (ductile) iron | When to choose |
|---|---|---|---|---|
| Sand, hand moulded | DCTG 11–14 | DCTG 11–14 | DCTG 11–14 | Large or low-quantity parts; machining allowance absorbs variation |
| Sand, machine moulded | DCTG 8–12 | DCTG 8–12 | DCTG 8–12 | Repeat production of small and medium parts |
| Shell moulding | DCTG 8–11 | DCTG 7–10 | DCTG 7–10 | Thin walls, better surface, closer as-cast sizes |
| Investment casting | DCTG 4–6 | DCTG 4–6 | DCTG 4–6 | Small precision parts with little machining |
Ranges are typical values taken as general guidance from the informative annex of ISO 8062-3; the grade for your part is agreed with the foundry after drawing review.
How to use the matrix: 1) pick the process your quantity and size allow; 2) read the typical DCTG for your metal; 3) write the grade and the machining allowance grade (RMAG) in the drawing title block; 4) mark tighter tolerances only on functional dimensions.
Quotable: “Tolerance grade follows process first: choose the moulding route, then write the DCTG it can hold.”
Related: machining allowance on castings.
Next step: Send your drawing for a technical review or request a metallurgy consultation at info@alloynex.com. State grade, size, quantity, tests and delivery town.
Last updated: 15 Nov 2026
ISO 8062-3 DCTG grades: myths vs facts
Short answer: DCTG grades in ISO 8062-3 run from 1 (tightest) to 16 (widest), and the table value is the total tolerance band, not a plus-minus value. Grey iron, SG iron and steel sand castings usually hold DCTG 8 to 12 when machine moulded and DCTG 11 to 14 when hand moulded. The myths below cause most drawing disputes.
| Myth | Fact |
|---|---|
| “DCTG 10 means ±3.6 mm.” | The table value is the total band. Split it in half for a symmetrical tolerance. |
| “A tighter DCTG always gives a better casting.” | A grade tighter than the moulding process can hold only adds rework and rejections. Match the grade to the process. |
| “CT grades and DCTG grades are different systems.” | CT came from ISO 8062:1994. ISO 8062-3 renamed them DCTG and kept the same numbering. |
| “ISO 2768 general tolerances can cover cast faces.” | ISO 2768 is for machined features. As-cast faces need an ISO 8062-3 note. |
| “Wall thickness follows the general DCTG.” | For walls, the standard applies one grade coarser (for grades up to DCTG 15). |
| “Machining allowance and DCTG are the same thing.” | RMA is extra metal for machining; DCTG is the permitted size variation. Both appear in the note. |
A clear drawing note: “General tolerances ISO 8062-3 – DCTG 11 – RMA 5 (RMAG H). Machined features to ISO 2768-m.” Put tighter tolerances only on the few dimensions that need them.
Read next: machining allowance on castings and design tips for better castings. Send your drawing for a technical review to info@alloynex.com.
Last updated: 15 November 2026
ISO 8062-3 on drawings: 7 mistakes to avoid
Most casting tolerance disputes start on the drawing, not in the foundry. The seven mistakes below cause good castings to be rejected or bad ones to be accepted. Each has a one-line fix that a design engineer can apply before the drawing is released for an enquiry.
Last updated: 16 Nov 2026
| # | Mistake | What goes wrong | Fix on the drawing |
|---|---|---|---|
| 1 | No casting tolerance note at all | Each side assumes a different grade | Title block note: General tolerances ISO 8062-3 – DCTG 11 – RMA grade |
| 2 | ISO 2768 on as-cast faces | Machining tolerance applied to raw surface; good castings rejected | ISO 2768 only on machined features |
| 3 | Reading the DCTG value as plus-minus | Tolerance doubled by mistake | Remember the table value is the total band; 5.0 mm means ±2.5 mm |
| 4 | Same grade for walls and outer sizes | Wall checks fail on sound castings | Walls take one grade coarser, as ISO 8062-3 allows |
| 5 | Ignoring the parting line | Mismatch and extra thickness across the joint | Show the parting line or let the foundry propose it at review |
| 6 | No machining allowance for machined faces | Faces clean up short and leave black spots | Write the RMA grade, e.g. RMAG H, and mark machined faces |
| 7 | Tighter grade than the process can hold | Higher cost and rejections with no benefit | Hand moulding usually DCTG 11 to 14; machine moulding DCTG 8 to 12 |
Fact: a 120 mm as-cast size at DCTG 11 has a 5.0 mm total band, so it may measure 117.5 to 122.5 mm.
Related: FG 260 grey iron castings for Sikar buyers · marble machinery castings in Kishangarh · machining allowance on castings
Send your drawing for a technical review and the tolerance note will be checked against the moulding method: info@alloynex.com.
Related: flywheel castings for Alwar buyers: FG 260 or SG 500/7